 A Guide to Problem Solving - The Application of Interior Wood Coatings
You got here from Home/Group/English/PRODUCTS/Problem Solving Guide
Flow
The ability of the coating to flow out to a uniform thickness after application, lack of flow is apparent when an uneven appearance results.
Cause
Preventative Action
Coating viscosity too high.
Apply all Mirotone coatings at the viscosity detailed in the relevant product data sheet.
Use of incorrect thinners.
Use only the correct MIROSOL thinner as specified on the product data sheet.
Poor fluid atomisation from spray gun.
Adjust spray gun settings to achieve correct fluid atomisation. Contact your Mirotone representative if problem persists.
Film weight too thin.
Apply all Mirotone coatings to the correct Wet Film Thickness as per instructions on the relevant product data sheet.
Draught conditions in spray booth and drying rooms.
Ensure spray booths and drying rooms have adequate but not excessive ventilation. A maximum airflow of 0.5m³ per second is recommended.

Back to Problem Solving Guide

Disclaimer: The recommendations above are based on data from Mirotone’s own research and information from others whose work we believe to be reliable. Due to possible differences in actual application methods and conditions, users must satisfy themselves that the end result meets their requirements.
     
 
Home | About Us | Site Map | Privacy | Disclaimer | Contact Us
2005 Copyright Mirotone

Content Management and Software Development by Elcom Technology